            基本信息:
            分類 種類 型號 標準 國家 應用
            Steel Grades - X20Cr13
            化學成分信息(mass fraction)(wt.%) of the X20Cr13
            元素名稱 最小值 最大值 近似值
            Cr 12.0000 14.0000 -
            P - 0.0451 -
            S - 0.0300 -
            Mn - 1.0000 -
            Si - 1.0000 -
            C 0.1700 0.2500 -
            Si - 1.0000 -
            S - 0.0300 -
            P - 0.0400 -
            Mn - 1.5000 -
            Cr 12.0000 14.0000 -
            C 0.1600 0.2500 -
            Si - 1.0000 -
            S - 0.0150 -
            P - 0.0400 -
            Mn - 1.5000 -
            Cr 12.0000 14.0000 -
            C 0.1600 0.2500 -
            Al 0.1000 0.3000 -
            Si - 1.0000 -
            S - 0.0300 -
            P - 0.0400 -
            Mn - 1.5000 -
            Cr 12.0000 14.0000 -
            C 0.1600 0.2500 -
            Si - 1.0000 -
            S - 0.0150 -
            P - 0.0400 -
            Mn - 1.5000 -
            Cr 12.0000 14.0000 -
            C 0.1600 0.2500 -
            Si - 1.0000 -
            S - 0.0150 -
            P - 0.0400 -
            Mn - 1.5000 -
            Cr 12.0000 14.0000 -
            C 0.1600 0.2500 -
            Si - 1.0000 -
            S - 0.0300 -
            P - 0.0400 -
            Mn - 1.5000 -
            Cr 12.0000 14.0000 -
            C 0.1600 0.2500 -
            Si - 1.0000 -
            S - 0.0150 -
            P - 0.0400 -
            Mn - 1.5000 -
            Cr 12.0000 14.0000 -
            C 0.1600 0.2500 -
            機械性能信息:
            屈服強度Rp0.2(MPa) 抗拉強度Rm(MPa) 沖擊率 伸長率 斷面收縮率 熱處理狀態 布氏硬度(HBW)
            128 (≥) 115 (≥) 44 12 42 Solution and Aging, Annealing, Ausaging, Q+T,etc 342
            物理性質信息:
            溫度 彈性模量 系數 熱導率 比熱容量 比電阻率 密度 加權系數
            12 - - 0.11 -
            722 417 - 41.3 431 -
            919 - 34 21.2 331 232
            熱處理信息:
            Heat treated : 1252°C - 1823°C
            對照表(同等等級)信息:
            型號 標準 國家 應用
            Y1Cr18Ni9 Improve the machinability, ablation resistance. Suitable for automatic lathe production of bolt and nut
            1Cr18Ni9 High strength after cold forming, but elongation than 1 cr17ni7 slightly worse. Used in architectural decoration parts
            1Cr18Mn10Ni5Mo3N Of urea with good corrosion resistance, can produce urea corrosion of the equipment.
            1Cr17Ni7 High strength after cold forming. Used in railway vehicle, conveyor belt, bolt and nut, etc
            Y1Cr18Ni9Se Improve the machinability, ablation resistance. Suitable for automatic lathe production of rivets, screws
            0Cr18Ni9 Seamless stainless steel tubes for boiler and heat exchanger
            00Cr19Ni10 Carbon content lower than 0Cr19ni9 steel, excellent intergranular corrosion resistance, is used for welding after the class is not processed parts
            1Cr17Mn6Ni5N Nickel steel grade, instead of number 1 cr17ni7 and magnetism after cold working, used in railway vehicle, etc
            1Cr18Mn8Ni5N Nickel steel, instead of 1cr18ni9
            0Cr19Ni9N Based on 0cr19ni9 plus N, strength increase and the plastic is not down. Reduce the thickness of the material. As a structure with strength components
            0Cr19Ni10NbN Based on zero cr19ni9 plus N and Nb, with better than 0 cr19ni9 properties and USES
            00Cr18Ni10N In 00cr19ni10 adding N, on the basis of the above grades also features, use the same as the 0 cr19ni9n, but better intergranular corrosion resistance
            1Cr18Ni12 Compared with 0 cr19ni9, processing low hardenability. Used for spinning processing, special drawing, cold heading
            0Cr23Ni13 Corrosion resistance and heat resistance are better than 0cr19ni9
            0Cr25Ni20 Oxidation resistance is better than 0cr23ni13. Mostly used as heat resistant steel
            0Cr17Ni12Mo2 Seamless stainless steel tubes for boiler and heat exchanger
            1Cr18Ni12Mo2Ti Seamless stainless steel tubes for boiler and heat exchanger
            0Cr18Ni12Mo2Ti Seamless stainless steel tubes for boiler and heat exchanger
            A-29 1025 General use carbon steel rod
            1025 These products have been used typically for use in fabrication of fittings, but usage is not limited to such applications. These products are not typically used for deep forming or cupping operations.
            標簽: X20Cr13、X20Cr13鋼材、X20Cr13材料
            全球鋼材百科網
            主站蜘蛛池模板: 日本高清视频色wwwwww色| 中文在线视频观看| 色九月亚洲综合网| 怡红院亚洲红怡院在线观看| 亚洲成av人片在线看片| 色噜噜狠狠狠狠色综合久一| 国产视频一二区| 久久精品无码一区二区三区| 欧美精品久久天天躁| 国产欧美日韩va另类在线播放| 久久久久噜噜噜亚洲熟女综合| 狠狠躁夜夜躁人人爽天天天天97 | 亚洲国产超清无码专区| 男人扒女人添高潮视频| 国产亚洲美女精品久久| 2021国产麻豆剧传媒官网| 在线观看污视频网站| 亚洲AV无码潮喷在线观看| 精品久久中文字幕有码| 国产精品入口免费麻豆| 久久99精品国产麻豆不卡| 欧美换爱交换乱理伦片老| 国产亚洲综合一区二区在线| 91精品国产高清91久久久久久 | 国产又黄又刺激又爽视频黄| 一本色道无码道dvd在线观看| 最近电影在线中文字幕| 又黄又爽又色的黄裸乳视频| 999精品视频在线观看热6| 无码中文资源在线播放| 人人揉人人爽五月天视频| 里番本子库全彩acg亚洲| 国产精品福利自产拍在线观看| 久久久无码精品午夜| 欧美精品videosex极品| 北条麻妃久久99精品| 高清亚洲综合色成在线播放放| 女神校花乳环调教| 亚洲AV成人片色在线观看高潮 | 最近更新中文字幕在线| 亚洲精品中文字幕麻豆|